1. Imilinganiselo ecetyiswayo yeZithinteli zomlilo

I-Aluminium Hypophosphite

  • Idosi:5%–10%
  • Umsebenzi:Isebenza kakuhle kakhulu ekuthinteleni ilangatye, ikhuthaza ukwakheka kwetsha, kwaye inciphisa izinga lokukhululwa kobushushu.
  • Phawula:Ubuninzi obugqithisileyo bunokuphazamisa ukuguquguquka kwezinto; kufuneka kufakwe izinto ezisebenzisanayo ukuze kuphuculwe umgangatho.

I-MCA (iMelamine Cyanurate)

  • Idosi:10%–15%
  • Umsebenzi:I-gas-phase flame retardant, ifunxa ubushushu kwaye ikhuphe iigesi ezingasebenziyo (umz., i-NH₃), isebenzisana ne-aluminium hypophosphite ukuphucula i-flame retardant.
  • Phawula:Ukulayisha kakhulu kunokubangela ukufuduka; kufuneka kuqinisekiswe ukuba kuyahambelana ne-EVA.

I-Magnesium Hydroxide (Mg(OH)₂)

  • Idosi:20%–30%
  • Umsebenzi:Ukubola kwe-endothermic kukhupha umphunga wamanzi, kunyibilikise iigesi ezivuthayo kwaye kuthintele umsi.
  • Phawula:Umthwalo ophezulu unokunciphisa iipropati zoomatshini; kucetyiswa ukuba kutshintshwe umphezulu ukuze kuphuculwe ukusasazeka.

2. Iingcebiso zokuphucula ukwenziwa kwefomyula

  • Inkqubo Ethintela Ilangatye Iyonke:Akufuneki kudlule i-50% ukulinganisela ukungabikho kokukhanya kwelangatye kunye nokukwazi ukulisebenzisa (umz., ukuguquguquka, izinga lokuncipha).
  • Iziphumo zokusebenzisana:
  • I-aluminium hypophosphite kunye ne-MCA zinokunciphisa iidosi nganye nganye (umz., i-8% ye-aluminium hypophosphite + 12% ye-MCA).
  • I-Magnesium hydroxide incedisana nokungavuthi komlilo ngokusebenzisa iziphumo ze-endothermic ngelixa inciphisa umsi.
  • Unyango Lomphezulu:Iiarhente zokudibanisa i-silane zinokuphucula ukusasazeka kunye nokubopha kwe-interfacial ye-magnesium hydroxide.
  • Izongezo eziNcedisayo:
  • Yongeza ii-2%–5% zezinto ezenza i-char-forming agents (umz., i-pentaerythritol) ukuphucula uzinzo lwe-char layer.
  • Faka izixa ezincinci zeeplastiki (umz., ioyile yesoya efakwe i-epoxidized) ukuze kulungiswe ukulahleka kokuguquguquka.

3. Imiyalelo yoQinisekiso lokuSebenza

  • Uvavanyo lokuBuyiselwa yiLanga:
  • Uvavanyo lokutshisa oluthe nkqo lwe-UL94 (ithagethi: V-0).
  • Umlinganiselo we-Oxygen Index (LOI >28%).
  • Iipropati zoomatshini:
  • Hlola amandla okuxinana kunye nobude ngexesha lokuphumla ukuqinisekisa ukuba ukuguquguquka kuyahlangabezana neemfuno zesicelo.
  • Ukuqhubekeka:
  • Jonga iMelt Flow Index (MFI) ukuze uphephe ubunzima bokucubungula ngenxa yokugcwala kakhulu kwezinto ezizalisa amanzi.

4. Iingqwalasela zeendleko kunye nokusingqongileyo

  • Ibhalansi yeendleko:I-aluminium hypophosphite ibiza kakhulu; idosi yayo ingancitshiswa (yongezwe nge-MCA) ukulawula iindleko.
  • Ubuhlobo nokusingqongileyo:I-Magnesium hydroxide ayinabungozi kwaye ithintela umsi, nto leyo eyenza ukuba ifaneleke ukusetyenziswa ngendlela enobuhlobo nokusingqongileyo.

Umzekelo Wokwenziwa (ngokwereferensi kuphela):

  • I-Aluminiyam Hypophosphite: 8%
  • I-MCA: 12%
  • I-Magnesium Hydroxide: 25%
  • I-EVA Matrix: 50%
  • Ezinye izongezo (ii-coupling agents, ii-plasticizers, njl.njl.): 5%